For any light below 350 nm, use fused silica: about 90 % transmission at 254 nm with a 180 nm cutoff, against under 10 % at 300 nm for borosilicate 3.3. Above 400 nm the two differ by less than 2 %, and a borosilicate window costs roughly a quarter as much.
Borosilicate glass is not "UV transparent with a small loss". At 1 mm thickness it holds 91 % at 365 nm, falls to 84 % at 334 nm, and is down to a few percent at 300 nm with a 50 % point near 310–320 nm. Fused silica at the same thickness holds 92 % at 365 nm, 90 % at 254 nm and is still above 80 % at 200 nm. Soda-lime glass, sometimes substituted, cuts off near 350 nm and should not see any UV source.
The practical question is whether your catalyst absorbs in the window's dead band. Anatase TiO2 has a 3.2 eV gap, an absorption edge at 388 nm, and works fine behind borosilicate. A wide-gap oxide such as ZnGa2O4 (4.5 eV, 276 nm) or a 254 nm low-pressure mercury lamp does not: behind 3 mm of borosilicate the 254 nm line is extinguished and the experiment returns zero.
The 300–320 nm slice that borosilicate removes carries roughly 10–15 % of a xenon lamp's 300–400 nm output, and under 1 % of total AM1.5G power. For a 388 nm edge that loss is small; for a 350 nm edge it is a large fraction of the useful photons.
| Property | Borosilicate 3.3 | Fused silica (UV grade) | Consequence |
|---|---|---|---|
| Internal transmission, 1 mm | 91 % at 365 nm / <10 % at 300 nm | 92 % at 365 nm / 90 % at 254 nm | Decisive below 350 nm |
| 50 % cutoff | 310–320 nm | 160–180 nm | Hg 254 nm needs silica |
| Refractive index, 589 nm | 1.47 | 1.46 | 4 % Fresnel loss per face, both |
| CTE, 20–300 °C | 3.3 × 10-6 /K | 0.55 × 10-6 /K | 6× difference in thermal stress |
| Safe thermal shock | about 100 K | about 800 K | Quartz survives a cold splash |
| 185 nm transmission | blocked | passed | Ozone risk only with silica |
| Relative cost, same size | 1 | 4–8 | Silica only where it earns it |
Values are internal transmittance for polished 1 mm sheet; a 5 mm window loses another 2–4 % at 365 nm, so specify thickness with material.
Apparent quantum yield shifts with the window. Swap borosilicate for silica on a 365 nm LED system and transmitted flux rises 1–2 %, since both are near 90 % there. Swap it on a mercury system whose 313 nm line dominates and the flux can rise by a factor of two. Any AQY change after a window replacement should be checked against a measured irradiance, never assumed.
Ozone is a silica-only problem. Low-pressure mercury lamps emit at 185 nm as well as 254 nm, and 185 nm photolyses O2 into ozone at a quantum yield near 2. A borosilicate window blocks 185 nm and keeps the bench breathable; a silica window does not, so it needs an enclosure or an ozone filter. The same 185 nm is what ages silicone seals and fogs up nearby optics.
Alkali leaching moves the pH. Borosilicate releases sodium and boron into alkaline slurry, and a 24 h run at pH 11 can drift the solution by 0.2–0.5 units, which matters when the reaction itself is pH sensitive. Fused silica leaches an order of magnitude less. If you run basic conditions with a sacrificial agent, either use silica or measure pH before and after.
Borosilicate can be flame-sealed to matching glassware, is tougher under point loads, and far more forgiving to machine and replace. A scratched silica window propagates a crack from a small flaw; borosilicate usually chips and stops. For a routine 365 nm or 405 nm screening reactor the optical penalty is 1–3 %, and the replacement cost after a student drops a cell is a fifth as much.
Pressure is usually not the deciding factor at laboratory scale. For a 50 mm clear aperture at 0.1 MPa gauge, a 5 mm borosilicate disc sits near 2 MPa bending stress, four times below its design strength; silica is stronger but notch-sensitive at the seal groove. Above 0.5 MPa the window becomes a pressure boundary and belongs to a rated design, not a catalogue disc.
Yes for anatase TiO2 under 365 nm or 405 nm LEDs, where the 388 nm absorption edge sits well inside the transmission band and the loss is 1 to 3 %. No for any system driven by a 254 nm mercury lamp or a catalyst with an edge below 350 nm, where the window removes most of the useful photons.
Borosilicate 3.3 reaches 50 % transmission near 310 to 320 nm and is effectively opaque at 254 nm. UV-grade fused silica reaches 50 % near 170 nm and still transmits about 90 % at 254 nm. The gap between the two curves is the entire 250 to 320 nm region.
Only if the lamp emits at 185 nm, as low-pressure mercury lamps do. Fused silica passes 185 nm, which splits O2 into ozone; borosilicate blocks it. Either enclose the lamp or fit an ozone filter when using silica with such a lamp.
Both add about 4 % reflection per face and a small absorption, but borosilicate adds a wavelength-dependent loss that your meter will not see if it is calibrated at 365 nm while your catalyst absorbs at 320 nm. Measure with the window in place, or correct by the measured transmission at the lamp line.