Fit rate against irradiance as r = k Iα across at least five points spanning one decade. A 1 g L−1 TiO2 slurry gives α = 0.7–1.0 below about 20 mW cm−2 and 0.5–0.6 above 50 mW cm−2, where recombination becomes second order. A 20 % lamp decay therefore costs 20 % of rate at α = 1 but only 11 % at α = 0.5.
Absorption generates electron–hole pairs at a rate proportional to the local photon flux, so the generation term G scales linearly with I. What happens next sets the exponent. At low intensity, carriers recombine mainly through first-order trap pathways, so the steady-state carrier density n is proportional to G and the surface reaction rate is proportional to I. The measured order is 1.0.
At higher intensity, the trap density is saturated and recombination becomes bimolecular: two carriers must meet, giving a loss rate k2n2. With equal electron and hole densities, G = k2n2, so n scales as I0.5 and the rate inherits the half order. The crossing point sits where k1n = k2n2, which for anatase in a typical slurry falls between 5 and 50 mW cm−2, depending on trap density, film thickness and sacrificial agent.
The consequence is arithmetic. If the lamp loses 20 % of its output over 500 h, a half-order system loses 11 % of its rate. Read against the initial measurement, that looks like deactivation, and no amount of XRD or BET will explain it.
Use one lamp and a set of neutral-density filters: switching lamps changes the spectrum, whereas filters attenuate without moving the emission lines. The filters must be UV-grade fused silica, mounted before the reactor window, with transmission measured at the lamp's peak wavelength rather than taken from a catalogue.
| Nominal OD | Transmission at 365 nm | Irradiance from a 100 mW cm−2 source | Notes |
|---|---|---|---|
| 0 | 100 % | 100 mW cm−2 | Reference point, measure each session |
| 0.1 | 79 % | 79 mW cm−2 | Small step, useful at the top end |
| 0.3 | 50 % | 50 mW cm−2 | Stable, low fluorescence |
| 0.5 | 32 % | 32 mW cm−2 | Heats by 3–8 °C under 300 W lamps |
| 0.7 | 20 % | 20 mW cm−2 | Transition region for most slurries |
| 1.0 | 10 % | 10 mW cm−2 | Cool the filter or use a larger aperture |
| 1.5 | 3.2 % | 3.2 mW cm−2 | Approaching the detection limit for products |
| 2.0 | 1 % | 1 mW cm−2 | Only with sensitive gas analysis |
Keep the illuminated area and loading fixed while changing filters, and measure irradiance at the reactor window plane with the same meter used for the reference point: a 10 % error on that axis shifts the fitted slope by about 0.04.
| Apparent α | Regime | What limits the rate | What to check |
|---|---|---|---|
| 0.9–1.1 | Photon-limited | Every absorbed photon is used | Product detection limit, not kinetics |
| 0.6–0.9 | Transition | Mixed first- and second-order recombination | Fit range too narrow to separate regimes |
| 0.45–0.6 | Recombination-limited | Bimolecular carrier loss | Normal behaviour above 50 mW cm−2 |
| 0.2–0.4 | Site or mass-transfer limited | Active sites, adsorption, diffusion | Loading, mixing, catalyst film thickness |
| <0.2 | Transport-limited | Product removal or light penetration | Slurry concentration, path length |
An exponent above 1.1 is almost never kinetics. It usually means the reactor heated up as the intensity rose, or that the irradiance was measured at a plane different from the one the catalyst sees. Both are worth ruling out before reporting a super-linear response.
Fix everything except intensity. Temperature to ±0.5 °C, catalyst loading in g L−1, sacrificial agent concentration, stirring rate and gas flow. Photocatalytic rates carry an apparent activation energy of 20–60 kJ mol−1, so a 10 °C rise between the lowest and highest intensity points can add a factor of 1.3–2.0 and bend the fit upward.
Take five points, wait for steady state at each. Ten to twenty minutes per point is typical for a slurry, less for a fixed bed. Run the series low to high and back once, and discard points that do not reproduce within 5 %.
Fit in log space. A least-squares fit of log r against log I gives α directly, with a standard error below ±0.05 over a decade. Report the fit range, r2 and the irradiance of every point.
Report apparent quantum yield at a stated intensity. AQY is not a material constant: it falls as intensity rises, because the same recombination that produces the half order wastes an increasing fraction of absorbed photons. Quote AQY at the irradiance used, or use the low-intensity plateau where α is close to 1.
Lamp aging. A 300 W xenon lamp loses 20–30 % of its UV output over 500–1000 h. At α = 0.5 the rate falls 11–16 %, which a cycling study reports as deactivation unless lamp hours are logged and intensity is re-measured at each run.
Photothermal heating. Above 100 mW cm−2, a dark slurry can rise 5–15 °C without a thermostat. That temperature gain is added to the intensity response, the fitted exponent climbs above 1, and the result gets read as cooperative photocatalysis.
Loading effects. At 2 g L−1 and a 10 mm path, most light is absorbed in the first 100 µm, so the volume-averaged rate saturates earlier and the apparent exponent drops to 0.3–0.4. That is a light-penetration number, not a catalytic one.
Because at high intensity the dominant loss is bimolecular recombination of electrons and holes. With equal carrier densities, the generation rate equals k2n2, so n scales as the square root of I and the surface reaction, which is first order in carriers, inherits the half order.
At least five, spanning a full decade, with a fitted standard error below ±0.05 and r2 above 0.99. Three points over a factor of two will fit any slope between 0.3 and 1.5 and cannot distinguish the regimes in the table above.
Yes. Higher loading absorbs the light in a thinner layer, so the volume-averaged rate saturates at lower incident intensity and the apparent exponent falls, often to 0.3–0.4 at 2 g L−1 in a 10 mm path. Always report loading and path length with the fitted value.
Only after normalising. Convert each rate to an apparent quantum yield at its own irradiance, or rescale with the reported exponent. Comparing 10 mW cm−2 with 200 mW cm−2 can show a 4–6 fold gap with no difference in material quality.